Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Archive of useful information. This is not a discussion area.

Re: Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Postby ZapPat » Sat Mar 07, 2009 8:30 am

liveforphysics wrote:I'm going to send you regular cheap zippy 5Ah LiPo cells soldered together to be a single 10Ah cell.

We can see if you can find any measureable voltage drop with just a 35amp load :)

Then you can calculate energy and energy density so people can see what the lure of the "darkside" battery chemistry is all about, :twisted:

I picked up five zippy flightmax 15C packs when you pointed out the special a couple weeks ago, and I am very impressed by them so far.

Here's a picture of one pack (5 cells, 18.5V nominal, 5Ah), and it measures 145mm X 40mm X 50mm:
Zippy LiPo 15C flighmax 5Ah, 5 cell 18.5V nominal.jpg
Zippy LiPo 15C flighmax 5Ah, 5 cell 18.5V nominal.jpg (73.55 KiB) Viewed 2045 times

Since a lifebatt/PSI/BMI is about 140mm long X 38mm dia, this would mean that a LiPo pack made with these would be almost 2.5X more energy dense than a same sized PSI/etc pack! :shock:

GO Doc, Go!!! You really should consider changing your name to DocBatt after this, since your excellent comparison charts are certainly going to be used by many internet surfers everywhere to make enlightened battery choices.
Norco Atomik DH bike - 3p12s Lipo (44V/15Ah), 9C rear hub, infinion/XC116 moded 6 FET (IR4110's) controller ~40A limit
2WD trail bike - 3p12s Lipo, Dual 9C hubs on 20" rims, dual moded 12 FET (IR3006's) ~100A+, 16"X3" motocross tires - A tank!
2WD road bike - 6p12s Lipo, Dual 9C hubs on 26" rims, dual moded 6 FET (IR4110's) ~70A
User avatar
ZapPat
100 kW
100 kW
 
Posts: 1010
Joined: Sat Jun 28, 2008 1:24 pm
Location: Eastern Canada (Gaspésie)

Re: Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Postby TylerDurden » Sat Mar 07, 2009 8:37 am

ZapPat wrote:I picked up five zippy flightmax 15C packs when you pointed out the special a couple weeks ago, and I am very impressed by them so far.
Blue flames... truth in packaging. :D
Have a Nice Day,

TD

Image
___________________________________________________________

FYI: Adding pictures?

Bored?... take a crack at the unanswered posts

Please post your Watts-at-speed in the survey.



Image
User avatar
TylerDurden
100 GW
100 GW
 
Posts: 8540
Joined: Thu Jan 04, 2007 5:50 pm
Location: Wear the fox hat.

Re: Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Postby liveforphysics » Sat Mar 07, 2009 9:19 am

I'm glad you are enjoying those batteries :) Once you go LiPo, it's very tough to want to lug around anything else, and put up with wimpy discharge rates, battery heating, saggy voltage etc. Of course if your application requires a saftey chemistry, then you gotta pick from the saftey chemistry batteries.

And Fantastic work Doc! You are a major asset to not only this forum, but to people all around the world who have an interest in making battery powered devices. PM me your address.

Best Wishes,
-Luke
For ebike parts, don't be a douche, buy from http://www.ebikes.ca or http://www.MethTek.com

Justin saved the forum at great personal expense! The man is a legend and a hero!
User avatar
liveforphysics
100 GW
100 GW
 
Posts: 10967
Joined: Wed Oct 29, 2008 1:48 am
Location: Santa Cruz, CA, USA

Re: Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Postby ZapPat » Sat Mar 07, 2009 9:56 am

TylerDurden wrote:
ZapPat wrote:I picked up five zippy flightmax 15C packs when you pointed out the special a couple weeks ago, and I am very impressed by them so far.
Blue flames... truth in packaging. :D

That's a pheonix, though, TD, so it'll just fly right back out of those nice blue flames to live again and again... :wink:

I actually ran three series packs to the ground the other day (until the power level dropped almost all of a sudden to almost nothing), without a BMS or any cell-level LVC. I then thought about all the over-discharged Lipo stories, where they catch fire while charging afterwards. :| So I charged them up anyways of course, and low and behold they sucked in all their Amp-hours without a problem, and still work great. Here's a site with very good battery info; read the end of the linked page, under "Lithium Charged but Not Guilty?". It's good to be vigilant and fully aware of possible dangers as with anything, but remember that fear is a mind-killer.

Anyways, anyone wanting to read/post about modern LiPos can check this thread here, and keep Doc's batt test thread here relatively clean (hit me Doc): LiPoly evolves while LiFePO4 is stagnant?
Norco Atomik DH bike - 3p12s Lipo (44V/15Ah), 9C rear hub, infinion/XC116 moded 6 FET (IR4110's) controller ~40A limit
2WD trail bike - 3p12s Lipo, Dual 9C hubs on 20" rims, dual moded 12 FET (IR3006's) ~100A+, 16"X3" motocross tires - A tank!
2WD road bike - 6p12s Lipo, Dual 9C hubs on 26" rims, dual moded 6 FET (IR4110's) ~70A
User avatar
ZapPat
100 kW
100 kW
 
Posts: 1010
Joined: Sat Jun 28, 2008 1:24 pm
Location: Eastern Canada (Gaspésie)

Re: Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Postby Doctorbass » Sat Mar 07, 2009 1:25 pm

like i said to Phil, this morning it was 4:20am when i was still playing with some A123 for preparing for test compare

I took some of those...(please note they come from "deffective pack" that had few cell low)

and i did a discharge to test the RI with 10 in parallel... and:

:shock: I measured....

1 miliohm.. lol .. exactly the corresponding 10 miliohm per cell but with 10 in parallel..

I'll measure every single cell of these 10 cells (picked from 2 or 3 dewalt pack) and will choose the 5 bests.

then i'll parallel them and measure them.

The pack with 5 parallel cells i showed was made owth the deffective low cells took appart from the deffective pack.

I always keep these cells eventhou they have 1700 or 1900mAh.. The last time i measured it it had 8750mAh out of 5parallel low cells.

I plan to test it too and will compare low cells with good cells.. that will give us a real comparaison with bad and good cells

In fact i would almost call them bad cause they had less than 1V each when i took them appart.

I plan that i'll need 4 days to measure them.

results soon!

Thanks for yuor encouragement guys!.. (is that the good word?..) I often use Babelfish translatoe.. :oops:

Doc
________________
-Fastest speed record from now: 113 km/h measured on GPS
-Fastest ebike 106km/h on flat and managed to enter in the 19.875 sec on the 1/4 mile drag racing !
-0-70km/h in 5sec X5 5303 on 24"
TORQUE SETUP:
-Succeded to haul a 19200 pounds schoolbus!
-Team Konion Member
113kmh Giant___http://www.evalbum.com/3406
Mongoose____http://www.evalbum.com/1947
E-trike_______ http://www.evalbum.com/3776
http://twitter.com/DocbassMelancon
I speak FRENCH and english
User avatar
Doctorbass
100 GW
100 GW
 
Posts: 6527
Joined: Sun Apr 08, 2007 2:24 am
Location: Quebec, Canada East

Re: Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Postby Doctorbass » Sat Mar 07, 2009 1:38 pm

ZapPat wrote:GO Doc, Go!!! You really should consider changing your name to DocBatt after this, since your excellent comparison charts are certainly going to be used by many internet surfers everywhere to make enlightened battery choices.


Yeah.. that might be an idea since on google there is only 5 or 6 entry on that name...

But i dont know... it's been for long time i was called Doctorbass and that i adopted that name..

When i was almost playing with subwoofer and car audio amplifier few years ago, some friends called me that name and that continued for me.. that began on Dbdragracing website.. years 2000 or 1999 if i remember correctly..

I agree that ending doc with "bass" does less sens than batt..

but you guys what do you think..? does it really matter rebaptizing me? :|

... replacing 2 S with 2 T :lol:

:wink:



Doc
________________
-Fastest speed record from now: 113 km/h measured on GPS
-Fastest ebike 106km/h on flat and managed to enter in the 19.875 sec on the 1/4 mile drag racing !
-0-70km/h in 5sec X5 5303 on 24"
TORQUE SETUP:
-Succeded to haul a 19200 pounds schoolbus!
-Team Konion Member
113kmh Giant___http://www.evalbum.com/3406
Mongoose____http://www.evalbum.com/1947
E-trike_______ http://www.evalbum.com/3776
http://twitter.com/DocbassMelancon
I speak FRENCH and english
User avatar
Doctorbass
100 GW
100 GW
 
Posts: 6527
Joined: Sun Apr 08, 2007 2:24 am
Location: Quebec, Canada East

Re: Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Postby dnmun » Sat Mar 07, 2009 2:51 pm

stick with drbass, can you measure the internal resistance on the individual bad a123 cells with your mega charger thingy, before charging them up? and then later of course.
dnmun
100 GW
100 GW
 
Posts: 9161
Joined: Mon Jun 09, 2008 1:32 pm
Location: portland, or and loveland, co

Re: Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Postby Doctorbass » Sat Mar 07, 2009 7:39 pm

dnmun wrote:stick with drbass, can you measure the internal resistance on the individual bad a123 cells with your mega charger thingy, before charging them up? and then later of course.



i'll put that on the Biiiiiiig to do list

Doc
________________
-Fastest speed record from now: 113 km/h measured on GPS
-Fastest ebike 106km/h on flat and managed to enter in the 19.875 sec on the 1/4 mile drag racing !
-0-70km/h in 5sec X5 5303 on 24"
TORQUE SETUP:
-Succeded to haul a 19200 pounds schoolbus!
-Team Konion Member
113kmh Giant___http://www.evalbum.com/3406
Mongoose____http://www.evalbum.com/1947
E-trike_______ http://www.evalbum.com/3776
http://twitter.com/DocbassMelancon
I speak FRENCH and english
User avatar
Doctorbass
100 GW
100 GW
 
Posts: 6527
Joined: Sun Apr 08, 2007 2:24 am
Location: Quebec, Canada East

Re: Yesa vs Headway vs PSI vs Ebike.ca 12Ah LFP test graph

Postby oatnet » Sat Mar 07, 2009 10:43 pm

GGoodrum wrote:Pretty much all LiFePO4 cells have a "nominal" voltage of around 3.3V, and all optimally get charged to 3.65V.


That has been my experience, but I thought a read somewhere that LifeBatt was peak-charged 3.35v, must have been wrong. Since it is 3.65v, I am really suprised that the Lifebatt in Bob's graph discharged 20a at @ .1v lower than the Headway. Granted this is an original green cell, but still... Of course, the current PSI=LifeBatt that Doc tested discharges at higher voltage than the Headway, I guess that is the relevant comparison.

-JD
User avatar
oatnet
100 MW
100 MW
 
Posts: 2507
Joined: Thu Apr 26, 2007 3:03 pm
Location: SoCal, USA

Previous

Return to Technical Reference Area