going easy on the cell doesnt really improve its mah/cycle loss
trying higher amp discharge
ive set these settings by temperature
step 1- 90f/632mah 15amp
step 2- 101f/821mah 10amp
step 3- 103f/1271mah 7.5amp reached 103f and held steady
step 4- 99f/ 461mah 5amp
step 5- 96f/107mah 2.5amp
start of charge 86f
#214 d-3292, c-3226
#215 d-3281, c-3227
#216 d-3279, c-3224
#217 d-3278, c-3222
the numbers have stabilised
i went and re-read this thread, looked at the mah numbers
compared it to the 40T's numbers and theyre pretty close after 200 cycles
after the capacity test at 100 cycles, it looks like desulfating works
https://endless-sphere.com/forums/viewtopic.php?f=14&t=107573#p1577214
just didnt know what i was observing
will do another 100 cycles
#218 d-3276, c-3219
#219 d-3275, c-3218
#220 d-3274, c-3216
#221 d-3272, c-3217
#222 d-3272, c-3215
#223 d-3269, c-3210
had the cycle set for 9 and test had stopped, battery was 4.173v, gave it a charge and resumed test
#224 d-3283, c-3211
#225 d-3268, c-3212
#226 d-3269, c-3212
#227 d-3267, c-3210
#228 d-3265, c-3206
#229 d-3264, c-3206
#230 d-3263, c-3207
#231 d-3262, c-3206
#232 d-3259, c-3203
test stopped, battery was 4.169v charged to 4.2v
#233 d-3277, c-3202
#234 d-3258, c-3205
#235 d-3261, c-3207
#236 d-3263, c-3205
#237 d-3260, c-3202
#238 d-3260, c-3202
#239 d-3258, c-3204
#240 d-3257, c-3196
#241 d-3254, c-3196 each group of 9 cycles takes about 24hrs, ill keep giving it an hour break every 24hrs
charged battery
#242 d-3274, c-3194
#243 d-3249, c-3193
#244 d-3250, c-3194
#245 d-3248, c-3195
#246 d-3251, c-3193
#247 d-3250, c-3195
#248 d-3252, c-3197
#249 d-3251, c-3195
#250 d-3251, c-3200
1hr break and then top up charge
#251 d-3279, c-3194
#252 d-3250, c-3193
#253 d-3250, c-3192
#254 d-3247, c-3190
#255 d-3245. c-3190
#256 d-3248, c-3191
#257 d-3247, c-3192
#258 d-3248, c-3193
#259 d-3248, c-3191
1hr break/charge
#260 d-3271, c-3186
#261 d-3244, c-3188
#262 d-3245, c-3186
#263 d-3244, c-3187
#264 d-3244, c-3186
#265 d-3243, c-3188
#266 d-3245, c-3189
#267 d-3244, c-3185
#268 d-3242, c-3188
1hr break/charge
#269 d-3271, c-3187
#270 d-3242, c-3183
#271 d-3240, c-3184
#272 d-3240, c-3185
#273 d-3240, c-3185
#274 d-3241, c-3184
#275 d-3242, c-3187
#276 d-3241, c-3186
#277 d-3242, c-3185
1hr break/charge
#278 d-3263, c-3181
#279 d-3239, d-3181
#280 d-3238, c-3179
#281 d-3236, c-3181
#282 d-3236, c-3181
#283 d-3238, c-3179
#284 d-3236, c-3180
#285 d-3239, c-3182
#286 d-3239, c-3180
doing 0.8amp capacity test
d-3688, c-3541
#287 d-3296, c-3236
#288 d-3288, c-3229
#289 d-3281, c-3223
#290 d-3275, c-3217
#291 d-3270, c-3208
#292 d-3264, c-3206
#293 d-3260, c-3203
#294 d-3257, c-3201
#295 d-3258, c-3201
1hr break/charge
#296 d-3284, c-3193
#297 d-3251, c-3196
#298 d-3255, c-3196
#299 d-3251, c-3188
#300 d-3247, c-3188
#301 d-3245, c-3187
#302 d-3243, c-3185
1hr break/charge
going to cycle with no break between discharge/charge/cycle
#303 d-3265, c-3182
#304 d-3241, c-3184
#305 d-3239, c-3182
#306 d-3238, c-3183
#307 d-3240, c-3179
#308 d-3237, c-3178
#309 d-3236, c-3176
#310 d-3234, c-3176
#311 d-3231, c-3174
1hr break/charge need to do another 9 cycles to see/compare the numbers
#312 d-3252, c-3171
#313 d-3229, c-3172
#314 d-3228, c-3168
#315 d-3227, c-3170
#316 d-3228, c-3172
#317 d-3228, c-3170
#318 d-3229, c-3169
#319 d-3225, c-3167
#320 d-3225, c-3166
1hr break/charge- adding wait times in between dicharge/charge /cycle
#321 d-3253, c-3162
#322 d-3222, c-3162
#323 d-3219, c-3165
#324 d-3223, c-3164
#325 d-3221, c-3163
#326 d-3222, c-3164
#327 d-3223, c-3163
#328 d-3221, c-3163
#329 d-3222, c-1498 stopped test and put battery on shelf at 3.774v